Thixotropy in Thermal Paste and the Joint That Holds Its Height
Thixotropy Is the Hidden Specification: How Thermal Paste Holds a 20 µm Joint
Every thermal grease datasheet lists conductivity and impedance. Almost none lists how the material behaves in the ninety seconds between the squeegee leaving the stencil and the clamp closing. That interval is where bond line thickness is won or lost, and thixotropy is the property that governs it.
01 What thixotropy actually describes
A thermal paste is a suspension of ceramic particles in a silicone or synthetic carrier, and the particle network gives it a yield stress. Below that stress the material behaves like a soft solid; above it, the structure breaks and the material flows. Thixotropy adds a second dimension to that behaviour: the breakdown is time dependent and reversible. Shear it for a second and the viscosity falls; leave it alone and the network rebuilds over seconds to minutes, returning to something close to its original stiffness.
This distinction matters more than it looks in a thermal paste. A merely shear-thinning material — pseudoplastic — thins under shear and thickens instantly when the shear stops. A truly thixotropic thermal grease keeps thinning through the whole dispensing event, then takes a finite time to recover, and that recovery time is the material's most useful and least documented property. Too fast and the paste will not fill the aperture in the first place; too slow and a printed deposit slumps into a puddle before the assembly line closes the clamp.
02 Three regimes, three numbers
It helps to look at the thermal paste joint at three moments rather than one. At rest in the cartridge, the paste sees a shear rate below 0.1 s⁻¹. Passing through a stencil aperture at 30–50 mm/s, the local shear rate is in the 100–1,000 s⁻¹ range. After release, the deposit sits at effectively zero shear for seconds while the next operation catches up. Each regime asks for the opposite of the other two, and a thixotropic structure is what reconciles them.
| Regime | Shear rate | What the paste must do | Failure if it does not |
|---|---|---|---|
| At rest in the syringe | Under 0.1 s⁻¹ | Hold a yield stress, resist settling and drain | Oil separation, sedimentation, drip |
| Through the aperture or valve | 100–1,000 s⁻¹ | Drop viscosity, wet the surfaces, release cleanly | Short deposit, clogged aperture, stringing |
| After release, before clamp | Effectively zero | Rebuild structure fast, hold height and footprint | Slump, wet-out beyond the pad, uneven bond line |
The practical consequence of the third row is the one engineers underestimate. A 0.1 mm stencil that deposits 5.4 mg/cm2 has to still be 20 µm thick thirty seconds later, when the heatsink arrives. If the paste has slumped by 30 %, the clamp closes on the thicker centre and the edge stays dry, and the joint becomes a mixture of 30 µm and a contact gap — which no impedance figure on the datasheet will predict.
03 Quantifying it: the thixotropic index and the yield stress
Two measurements do most of the work for a thermal paste. The thixotropic index is the ratio of apparent viscosity at low shear to apparent viscosity at high shear, conventionally read at 1 s⁻¹ and 10 s⁻¹ on a rotational rheometer with a 20 mm plate. Proceedings-grade thermal greases typically land between 2 and 5; below 2 the material tends to drain and slump, above 6 it becomes difficult to print at 0.1 mm because it will not release from the aperture cleanly. The second measurement is yield stress, the stress at which the network collapses. Fifty to a few hundred pascals is the working range for a paste that must stay put on a vertical surface yet still be displaced by a 10–30 psi clamp.
Yield stress answers a question that viscosity cannot: will a bead of material sitting on a vertical inner wall stay there? For a film of thickness t on a vertical surface, gravity imposes a shear stress of roughly ρ g t. At 2.7 g/cm3 and a 0.3 mm layer that is about 8 Pa; at 1 mm it is 26 Pa. Both sit below the yield stress of a properly formulated thermal grease, which is why a paste does not creep down a wall the way a low-viscosity oil would. A material with a yield stress of 5 Pa, by contrast, will drain overnight, and the assembly will be found short of material at first power-on.
04 Why the joint survives thermal cycling
For a thermal interface material, the bond line is not static. A CPU lid and a heatsink expand at different rates, and the gap opens and closes by 5–15 µm on every power cycle. The thermal paste must accommodate that breathing without being squeezed out of the joint, which is the mechanism behind pump-out: low yield stress material migrates outward a few micrometres per thousand cycles until a dry ring forms at the edge and the centre carries all the load. Thixotropy is directly implicated, because recovery after each shear event is what keeps the material in place; a paste that recovers slowly behaves like a liquid at the joint and pumps out.
A second thermal paste failure runs the other way. In a gap that is 0.3 mm or wider, the thermal paste has to flow enough to fill the void, which needs a low enough yield stress and a shear-thinning profile. The same formulation property therefore has an upper and a lower bound, and the design target sits between them: enough structure to hold position and resist drain, little enough to fill a real gap at the pressure the assembly can apply.
05 Five ways thixotropy gets destroyed in production
- 01Diluting to make it printable. A splash of solvent drops the viscosity and makes a clogged stencil run again, but it also destroys the particle network. The paste prints beautifully and then slumps, outgasses at 80 °C, and leaves a 15 µm joint where 30 µm was designed.
- 02Choosing by viscosity alone. Two thermal pastes at 200 Pa·s can behave completely differently on a stencil, because one recovers in two seconds and the other in two minutes. Ask for the index and the recovery time, not the single viscosity figure.
- 03Re-stirring a settled cartridge. Long storage lets filler settle and oil separate; stirring restores the bulk but entrains air, and an air bubble in a 20 µm joint is a dry patch with a hotspot under it. Store flat, use date-coded cartridges, and degas before qualification.
- 04Qualifying at 25 °C only. Silicone carriers soften with temperature. A thermal paste with an index of 4 at room temperature may show 2.5 at 70 °C, and the difference is enough to turn a stable vertical joint into a slow drain over a two-year life. Measure at the operating temperature, not the lab temperature.
- 05Mixing two grades to stretch a batch. Two thixotropic structures do not average; they interfere. The mixture loses yield stress, slumps, and the resulting joint is worse than either component used alone.
06 Grades and the numbers behind them
The TSAD Series from TOUSEN is a solvent-free, non-curing, thixotropic grey thermal paste covering 1.2–6.5 W/m·K, with measured impedance of 0.030 to 0.201 °C·cm2/W at 30 psi, specific gravity 2.5–2.9 g/cm3, screen-printable consistency, low slump and a 12-month shelf life. Because the structure is designed for printing rather than for pouring, the grades with the highest filler loading remain printable at 0.1 mm even though their bulk conductivity has doubled.
| Grade | W/m·K | Impedance @ 30 psi (°C·cm2/W) | Density (g/cm3) | Where the structure matters most |
|---|---|---|---|---|
| TSAD60 | 1.2 | 0.201 | 2.5 | Thick gap fill, 0.2–0.3 mm, vertical walls |
| TSAD66 | 3.5 | 0.080 | 2.7 | 0.1 mm stencil, 20–40 µm, high volume |
| TSAD66-P | 4.0 | 0.070 | 2.6 | Rougher spreaders, thicker printed layer |
| TSAD83 PLUS | 5.2 | 0.050 | 2.6 | Jetting onto small, high-flux tabs |
| TSAD88 PLUS | 5.2 | 0.030 | 2.9 | Thin printed joint under a stiff clamp |
| TSAD90 | 6.5 | 0.030 | 2.7 | Multi-tab panels printed in one stroke |
| TSAD100 | 6.5 | 0.030 | 2.8 | Instrument coolers, thermal grease alternative |
The four questions worth asking a supplier
For a thermal interface material, conductivity is the easy number to publish and the least informative for a process engineer. A short list of rheology questions will separate a printable thermal grease from a thermal paste that merely looks printable on a datasheet.
| Property | How it should be measured | Working target |
|---|---|---|
| Thixotropic index | Apparent viscosity at 1 s⁻¹ over 10 s⁻¹, 25 °C | 2 to 5 |
| Yield stress | Controlled shear ramp, crossover point | 50 to 500 Pa |
| Slump after printing | 0.1 mm deposit, height at 10 and 30 min | Under 15 % loss |
| Oil separation | 150 °C, 24 h, weight loss or bleed ring | Grade-dependent, low |
07 What this changes in the design review
Thixotropy is not a marketing adjective; it is the mechanism that allows a thermal paste with a 20 µm working thickness to be applied at production speed and then stay where it was put. In practical terms it sets four limits: the thinnest layer a stencil can hold without slump, the widest gap a thermal paste can still fill at a given clamp pressure, the angle at which a joint can be mounted without draining, and the number of thermal cycles before the joint pumps out. All four appear in a thermal simulation as a single impedance number, which is why they are so often missed until the first field return.
For any thermal interface material, a supplier discussion should start with the index, the yield stress, the slump data and the impedance at the pressure your clamp actually delivers; the combination is a better guide to the finished joint than any conductivity figure. Grade tables, pressure-impedance curves and print trial samples for the TSAD thermal grease range are available on the TSAD Series thermal paste product page.
Thermal Paste Stencil Printing and Jetting Compared
Related Article